FREE WORKSHOP TOOL / 01

Filament drying table

Find source-specific temperatures and times. Follow the maker of your spool first, including the method and equipment it specifies.

Manufacturer drying guidance — choose the maker of your spool first
Material / productMakerMethod / settingTimeSource and limits
PLA
Prusament PLA / rPLA
PrusaFilament drying (see maker method)
45 °C
6 hPrusa guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

PETG
Prusament PETG (all versions)
PrusaFilament drying (see maker method)
55 °C
6 hPrusa guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

TPU
Prusament TPU
PrusaFilament drying (see maker method)
60 °C
4–6 hPrusa guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

ASA
Prusament ASA
PrusaFilament drying (see maker method)
80 °C
4 hPrusa guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

PC
Prusament PC Blend
PrusaFilament drying (see maker method)
85 °C
5 hPrusa guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

PC
Prusament PC Blend Carbon Fiber
PrusaFilament drying (see maker method)
90 °C
4 hPrusa guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

Nylon
Prusament PA11 Carbon Fiber
PrusaFilament drying (see maker method)
90 °C
6 hPrusa guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

PLA
PolyLite PLA
PolymakerFilament drying (see maker method)
55 °C
6 hPolymaker guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

PLA
PLA / PLA+
SUNLUFilament drying (see maker method)
50–55 °C
6–8 hSUNLU guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

PETG
PETG
SUNLUFilament drying (see maker method)
60–65 °C
6–8 hSUNLU guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

ABS
ABS
SUNLUFilament drying (see maker method)
75–85 °C
6–8 hSUNLU guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

ASA
ASA
SUNLUFilament drying (see maker method)
80 °C
6–8 hSUNLU guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

TPU
TPU
SUNLUFilament drying (see maker method)
50–60 °C
6–8 hSUNLU guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

Nylon
PA (Nylon)
SUNLUFilament drying (see maker method)
80–110 °C
4–12 hSUNLU guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

PC
PC
SUNLUFilament drying (see maker method)
70–80 °C
6–8 hSUNLU guidance
Checked 2026-10-25

Check the exact spool and filament limits before heating.

ASA
ASA Aero
Bambu LabForced-air drying (maker method)
80 °C
8 hBambu Lab guidance
Checked 2026-10-25

ASA Aero TDS states PC+ABS spool temperature resistance 90 °C. Printer-bed settings are specific to the documented X1 method, not chamber air.

ASA
ASA Aero
Bambu LabPrinter bed (documented setup only)
90–100 °C
12 hBambu Lab guidance
Checked 2026-10-25

ASA Aero TDS states PC+ABS spool temperature resistance 90 °C. Printer-bed settings are specific to the documented X1 method, not chamber air.

PVA
PVA (current quick-start guidance)
SUNLUFilament drying (see maker method)
50–60 °C
8–12 hSUNLU guidance
Checked 2026-10-25

Current SUNLU quick-start table differs from older indexed guidance. Check the exact product sheet and resolve conflicting instructions with SUNLU before heating.

Read a row before setting the heater

  1. Match the exact material and product. A reinforced blend may differ from the unfilled polymer.
  2. Open the maker's source and check its equipment, ventilation and spool instructions.
  3. Check that both your dryer and the spool are rated for the setting. More heat is not a substitute for the specified time.
  4. After drying, follow the maker's storage guidance. A dry box and a dryer perform different jobs.

Why don't all makers agree?

Filament formulations and drying equipment vary. We keep each maker's guidance separate rather than averaging it. A printer-bed surface setting cannot be substituted for a dryer's air setting.

Missing a maker? Send us its current technical document. We leave unverified settings out of this table.

Read the material guides →